ASTM A387锅炉容器板的化学成分:
ASTM A387 | UNS | C | Mn | P | S | Si | Cr | Mo | 其它 |
5级 | S50200 | ≤0.15 | 0.25-0.66 | 0.025 | 0.025 | ≤0.55 | 3.90-6.10 | 0.40-0.70 | - |
9级 | K90941 | ≤0.15 | 0.25-0.66 | 0.025 | 0.025 | ≤1.05 | 7.90-10.10 | 0.85-1.15 | *A |
11级 | K11789 | 0.04-0.17 | 0.35-0.73 | 0.025 | 0.025 | 0.44-0.86 | 0.94-1.56 | 0.40-0.70 | - |
12级 | K11757 | 0.04-0.17 | 0.35-0.73 | 0.025 | 0.025 | 0.13-0.45 | 0.74-1.21 | 0.40-0.65 | - |
22级 | K21590 | 0.04-0.15 | 0.25-0.66 | 0.025 | 0.025 | ≤0.50 | 1.88-2.62 | 0.85-1.15 | - |
22L级 | K21590 | ≤0.12 | 0.25-0.66 | 0.025 | 0.025 | ≤0.50 | 1.88-2.62 | 0.85-1.15 | - |
91级 | K90901 | 0.06-0.15 | 0.25-0.66 | 0.025 | 0.012 | 0.18-0.56 | 7.90-9.60 | 0.80-1.10 | *B |
*除非提供范围或另外指定,否则所有值均为下限值,并且应基于产品分析。
*A – V:≤0.05; B – Ni:≤0.43,V:0.16-0.27,Co:0.05-0.11,N:0.025-0.080,Al:≤0.02,Ti≤0.01,Zr≤0.01.
*A和*B中的所有值均应以“%”为单位。
ASTM A387锅炉容器板的力学性能:
ASTM A387 | 类别 | 抗拉强度 | 屈服强度 | 伸长率,标距2 in. [50 mm], % |
(Mpa) | (Mpa) | (%) | ||
5级 | 第1类 | 415-585 | 205 | 18 |
第2类 | 515-690 | 310 | 18 | |
9级 | 第1类 | 415-585 | 205 | 18 |
第2类 | 515-690 | 310 | 18 | |
11级 | 第1类 | 415-585 | 240 | 22 |
第2类 | 485-620 | 310 | 22 | |
12级 | 第1类 | 380-550 | 230 | 22 |
第2类 | 450-585 | 275 | 22 | |
22级 | 第1类 | 415-585 | 205 | 18 |
第2类 | 515-690 | 310 | 18 |
ASTM A387锅炉容器钢的对等材质:
(仅供参考)
美标 | 欧标 | 德标 | 英标 | 法标 | 俄标 | |
ASTM | ASME | EN 10028 | DIN | BS | AFNOR 36206 | GOST |
A387 5 | SA387 5 | X12CrMo5 | --- | --- | 15KH5M | |
A387 9 | SA387 9 | --- | --- | --- | ||
A387 11 | SA387 11 | 13CrMoSi5-5 | --- | 621B | ||
A387 12 | SA387 12 | 13CrMo4-5 | 13CrMo44 | 620B | 15CD2.05 | 12KHM |
A387 22 | SA387 22 | 10/11CrMo9-10 | 10CrMo9-10 | 622-515B | 12CD9-10 | 10KH2M |
A387 91 | SA387 91 | 10CrMoVNb9-1 | --- |
ASTM A387锅炉容器板中的钼成分可提高其在高温下的拉伸强度,并通过增加晶格应变使其具有较高的抗氧化和抗腐蚀能力。ASTM A387锅炉容器板是耐热压力容器和酸性气体环境下使用的理想选择。